Microstructural Development of Furan Resin by Hot-Pressing

Eiichi Yasuda, Yasuhiro Tanabe, Hiroshi Machino, Shiushich Kimura

TANSO · 1987 · 18 citations · 1 references

DOIFull text

Open access

Concepts

Abstract

Furan resin was hot-pressed at the temperature regions of curing, carbonization under the pressure of 2 to 82 MPa and further those were heat-treated at 3000°C.The resin pressed during carbonization was easily graphitized even under the pressing stress of 2 MPa.When the stress was supplied after carbonization at 1000°C, furan resin was also graphitized a little.However, the stress was much higher than that in the hot-pressing and was above 82MPa.After the resin began to be hard in curing, pressing as 82MPa dose not act on the graphitization of furan.

References

1