Advanced Materials · 2013 · 58 citations · 28 references
Natural SciencesMaterials EngineeringMaterials ScienceCatalysisMaterials ChemistryNanomaterialsEnergy ConversionMetal Oxide NanomaterialsNanocatalysisNanostructured Energy MaterialsOxygen EvolutionPhotocatalysisMetal-air BatteriesNanostructured PhotocatalystsOxygen Evolution CatalystsOxygen Evolution ReactionPhotocatalytic MaterialsPhotocatalytic Oxygen EvolutionPhotocatalytic Water SplittingWater Splitting
Uniformly cut In2O3 truncated octahedrons are fabricated on a large scale by a simple chemical vapor deposition (CVD) technique. This theoretical analysis predicts that the emergence of {100} facets on the In2O3 truncated octahedrons enhances oxygen evolution significantly in photocatalysis and experimental photoelectrochemical measurements are consistent. Photocatalytic water splitting by solar power is environmentally friendly and highly preferred.1 The oxygen evolution reaction (OER) is key to renewable-energy technologies such as rechargeable metal-air batteries2-4 and water splitting,5, 6 and water oxidation also plays an important role in energy storage such as solar fuel synthesis.7, 8 Despite extensive research, the effects of a catalytic surface on the OER are still not well understood9 and the development of economical oxygen electrode catalysts with high activity under visible-light irradiation remains a great challenge. Recently, Yang10 proposed that crystal cutting might increase the photocatalytic properties of materials such as Cu2O nanocrystals.11, 12 Although Cu2O delivers good performance in the photodegradation of methyl orange after crystal cutting,12 there has been no report on the direct photocatalytic water splitting into hydrogen or oxygen. In fact, surface oxidation of Cu2O to CuO introduces unstable photocatalytic characteristics in aqueous solutions after long-time irradiation.13 Markovic and co-workers reported enhanced hydrogen evolution from water splitting by tailoring the Li+(Ni(OH)2(Pt interfaces,14 but enhancement by crystal tailoring has not been reported. In this respect, it is crucial to develop crystal-cut photocatalytic materials with excellent oxygen evolution ability under visible-light irradiation and to elucidate the associated mechanism. In2O3 is a promising semiconducting material15-17 and has a bandgap of 2.8 eV. However, it has poor photocatalytic properties18 and no water splitting has been reported experimentally using In2O3 octahedron nanocrystals, although there has been litle theoretical work on water splitting on some special crystal facets.19 Here, we report a simple technique to produce uniformly cut In2O3 truncated octahedrons. Our theoretical analysis shows that the {100} facet on the In2O3 truncated octahedrons enhances oxygen evolution in photocatalysis and photoelectrochemical measurements provide the experimental evidence. In a body-center-cube (bcc) structural crystal such as Cu2O, the difference in the energy levels between the crystal faces can drive the photoexcited electrons and holes to different crystal faces, leading to the separation of electrons and holes. Previous investigation suggets that during irradiation by visible light, the photogenerated holes on the {111} facets will transfer to the {100} facets, whereas electrons on the {100} facets will migrate to the {111} facets.20 This is a prerequisite to the water-splitting reaction.7 The catalytic activity on the {111} facets stems from the Cu-terminated surfaces bonded with some stable groups.21 Hence, the electrically neutral {100} facets cannot interact well with charged molecules and is thus catalytically inactive.22 This implies that polar facets on the In2O3 crystal having the same crystal structure and adequate bandgap23, 24 as Cu2O may increase the photocatalytic activity in the water-splitting reaction. Figure 1a depicts the In2O3 octahedron24, 25 and Figure 1b–d show the atomic arrangements in a unit cell of the bcc structure along different lattice directions. The smaller and bigger spheres represent oxygen and indium atoms, respectively. The (002), (020), and (200) facets are arranged by the same type of atoms (indium or oxygen) as shown in Figure 1b,c. The distances between two adjacent facets are the same and they are the polar facets. The (220) and (222) facets, which have two different atoms (indium and oxygen) (Figure 1c,d), show electrical neutrality and are the nonpolar facets. a) Sketch of the In2O3 octahedron. b) A unit cell of the bcc structure viewed from the <220> direction with the lines representing the (002) facets. c) A unit cell of the bcc structure viewed from the <002> direction with the lines representing the (200), (020), and (220) facets. d) A unit cell of the bcc structure viewed from the direction parallel to the (222) facet with the lines representing the (222) facets. The spatial distributions of electron and holes excited by light irradiation on these crystal facets are theoretically investigated and the calculation details are described in Figure S1–S3 in the Supporting Information. The main panel in Figure S4a in the Supporting Information presents the densities of states (DOSs) of the bulk and slabs along the {100} and {111} directions of In2O3. Compared with the bulk materials and {111} surface, cleaving of the {100} surface creates a new valence subband (represented by peak A in the DOS) which is just below but very close to the Fermi level defined as the energy of the highest occupied state and set to zero energy. The spatial distribution of the orbital in this subband shown in the inset illustrates that the orbital is concentrated on the {100} surface. At the same time, the orbitals of the conduction band in both the {100} and {111} slabs are extended to the entire materials (see the Supporting Information). This implies that during light irradiation, the excited holes from valence sub-band A are concentrated on the {100} facets and the excited electrons are in the bulk. This produces a photoinduced dipole layer on the {100} facet, which may attract OH− groups from the solution. Such charge separation had been observed in small TiO2 particles based on density functional calculations.26 To investigate the effects of the {100} facets on H2O molecules, we perform geometry optimization on the {111} and {100} slabs with adsorbed H2O molecules. The optimized structures are shown in Figure S4b in the Supporting Information. On the {100} surfaces with and without induced charges, there are some H2O molecules that dissociate into H+ and OH−, whereas on the {111} surface, they cannot dissociate. The calculated DOS for the {100} slab with adsorbed H2O molecules is shown in Figure S5,S6 in the Supporting Information. Although there are some changes in detailed structures compared to that without H2O molecules, peak A which is responsible for the creation of holes still exists. Dissociation of H2O molecules on different surfaces has been investigated based on first-principle calulation.26-28 In this work, we perform geometry optimization for the surfaces with different H2O monolayer coverage from 1/8 to 1/2 and observe that 1/8 coverage is related to the dissociation for 1/2 water monolayer coverage on the {100} surface. Partial dissociation on the {100} surface may stem from the complicated In and O exposed structure. The calculation results also indicate that the {100} facets of In2O3 can effectively accumulate holes produced by light illumination, but on the nonpolar planes such as {222} and {220}, no corresponding process occurs. In an alkaline electrolyte, when there is an accumulation of holes (h+) on the surface, the In2O3 nanocrystal anode would undergo the following reaction: 4OH− + 4h+(VB) → O2↑ + 2H2O, cathode: 2H2O + 2e−(CV) → H2↑ + 2OH−.29-31 Hence, if the In2O3 nanocrystals with {100} facets are used as the anode, the photoexcited holes will transfer to the {100} surfaces to produce O2. This photo-electrochemical process will lead to effective oxygen evolution from the anode, thus providing a useful way to produce O2 based on crystal cutting. Since various crystal facets have different growth rates,25 the growth temperature and time must be tightly controlled in order to prepare In2O3 nanocrystals with the {100} surface exposed. The commonly fabricated In2O3 nanocrystals have the octahedral structure with the {111} surface for minimum surface free energy, and so the {100} In2O3 nanocrystals should be formed in the early stage. Details regarding the In2O3 nanocrystal growth process and mechanism are described in Figure S7 in the Supporting Information. By properly controlling the growth conditions, In2O3 octahedrons and truncated octahedrons with a uniform size can be produced in abundance, as shown in Figure 2a–d. Field-emission scanning electron microscopy (FE-SEM) reveals that the size of the truncated octahedrons is about 1 μm, which is almost equal to that of the octahedrons. Field-emission transmission electron microscopy (FE-TEM) images and selected area electron diffraction (SAED) patterns are acquired to confirm the observed different crystal facets. As shown in Figure 2e–g, the hexagonal symmetry diffraction spots are obviously observed from the (111) facets on the octahedron or truncated octahedron and meanwhile, the tetragonal symmetry diffraction spots arise from the (100) facets on the truncated octahedron (Figure 2h–j). The X-ray diffraction (XRD) patterns acquired from these In2O3 octahedrons and truncated octahedrons are displayed in Figure 2k. All the XRD peaks can be indexed to the (200), (211), (222), (400), (411), (440), (600), and (622) reflections of the bcc structure of In2O3 (according to the standard card of XRD, JCPDS card No. 06-416). In particular, the (222) peak from the octahedron sample is rather strong, but that from the truncated octahedron is relatively weak. The intensity of the (400) peak from the truncated octahedrons is enhanced. Although the XRD spectra are not related to the relative areas of the various crystal faces, considering the FE-SEM and FE-TEM results, it can be inferred that a large number of {100} facets are formed. According to the UV–vis diffusive reflectance spectra of the octahedron and truncated octahedron samples, the absorption curves are acquired and Figure S8 in the Supporting Information shows that the two kinds of octahedron samples have almost the same absorption features in the visible range. a) Low-magnification FE-SEM image of the octahedrons. b,c) Local enlargement (b) and low magnification (c) FE-SEM images of the truncated octahedrons. d,e) Local enlargement (d) and low-magnification (e) FE-TEM images of the octahedron. f) Sketch of octahedron viewed from the (111) facets. g) SAED pattern on the (111) facets. h) Low-magnification FE-TEM image of the octahedron. i) Sketch of the octahedron view from the (100) facets. j) SAED pattern acquired from the (100) facets. k) XRD patterns of the octahedron (upper curve) and truncated octahedron (under curve) samples. The photoelectrochemical measurements were performed in a three-electrode cell (Figure S9 in the Supporting Information) connected to a CHI 660D work station (CH Instrument) at ≈25 °C. The In2O3 nanocrystal sample with Ohmic contact served as the working electrode,32, 33 whereas Ag/AgCl (1 mol L−1 NaOH-filled) and a platinum wire were the reference and counter electrodes, respectively. The current–voltage (J−V) curves are shown in Figure 3. The circular, triangular, and quadrate curves are acquired from two In2O3 samples and a silicon substrate under illumination, respectively. The broken curve represents the cases for the octahedron, truncated octahedron, and silicon substrate samples without irradiation (dark). As the applied voltage is increased slowly from negative (−0.6 V) to positive (1.2 V), the broken curve is almost a straight line. Under Xe-lamp illumination, the photocurrent densities of both the octahedron sample and silicon substrate show little improvement compared with that without illumination, whereas that of the truncated octahedron sample (triangular curve) largely surpasses those of the octahedron sample and silicon substrate. To rule out that the rapid increase of the photocurrent density is due to different defect concentration, we mesaured the resistivity of the octahedron and truncated octahedron samples and the values are 353 and 578 mΩ cm, respectively. Hence, the truncated octahedron sample should have a smaller photocurrent, but our experimental results are not so, indicating that the {100} truncated octahedrons really have a high photocatalytic activity. Hence, the rapid increase indicates that the exposed truncated facets play an important role in the enhancement of the photocatalytic activity on the In2O3 nanocrystals. Current density versus applied potential curves of photoelectrochemical measurement. The circular and triangular curves are acquired from the two In2O3 samples with octahedron and truncated octahedron sizes of 1 μm, respectively. The quadrate curve is from the silicon substrate. The broken line represents the cases for the octahedrons, truncated octahedrons, and silicon substrate without irradaition (dark). To investigate the effective photocatalytic OER further, the applied voltage was fixed at 0.22 V versus Ag/AgCl and the photocatalytic current–time (I–t) curves are depicted in Figure 4. The triangular and circular curves are for the truncated octahedron and octahedron samples, respectively, under illumination, whereas the broken curve is acquired without illumination showing that no current is produced. During illumination, the photocurrent density measured from the octahedron sample is very small (0.04 mA cm−2), but that from the truncated octahedral sample is larger (1.4 mA cm−2) and remains stable during the entire observation time of 150 min. Almost no attenuation was observed, indicating both a robust and a stable photocatalytic activity. Two digital photos were taken from the truncated octahedral electrodes at 20 and 60 mins (an enlarged photo is shown in Figure S10 in the Supporting Information). In the initial stage, no bubbles were observed but as time elapsed, bubbles were produced gradually and they became bigger and bigger. In contrast, no bubbles could be observed from the solution surface with the octahedron electrode (lower inset). The amount of evolved O2 was calculated from the (I–t) curve and detected by a Shimadzu GC-8A gas chromatograph. The two sloping curves in Figure 4 show the theoretical and experimental results, respectively. It is obvious that the amount of evolved O2 increases with time and the experimental value is close to the theoretical one. In addition, the SEM image and XRD spectrum after the photoelectrochemical measurement confirm that the truncated octahedrons remain intact on the electrode (Figure S11 in the Supporting Information). These above provide experimental evidence that In2O3 possesses good photocatalytic characteristics after crystal cutting and it is consistent with the theoretical prediction described earlier. The truncated octahedrons have the advantage of multiple (100) facets being exposed to accumulate holes via photoexcited charge-carrier separation. This is responsible for the high photocatalytic activity. Furthermore, in comparison with Cu2O, the polar surfaces on In2O3 are stable in aqueous solutions and it is crucial to stable water splitting photocatalytically. Here, we would like to point out that the (100) facet is a polar surface and undergoes evident surface reconstruction in the aqueous environment (Supporting Information, Figure S4b), thereby improving the photocatalytical activity on the (100) facets further. Current density versus time curves and two digital photos for oxygen evolution. The triangular and circular curves are for the truncated octahedron and octahedron samples under illumination, respectively, whereas the broken curve is for the case without illumination. The upper insets show representative photocatalytic-oxygen-evolution photos of the truncated octahedron sample at different measurement times taken by a digital camera from the cell at an applied potential of 0.22 V (versus Ag/AgCl). No bubbles (oxygen evolution) are observed for the octahedron sample (lower insets). Two sloping curves show the amounts of evolved O2 calculated theoretically and detected experimentally, respectively. In conclusion, we have fabricated uniform truncated In2O3 nanocrystals on a large-scale on a silicon substrate using a simple technique. The experimental photocatalytic performance of the In2O3 truncated octahedrons is consistent with our theoretical prediction showing that the {100} truncated octahedrons have significantly improved photocatalytic activity compared with the octahedrons. The high photocurrent (1.4 mA cm−2, voltage = 0.25 V vs. Ag/AgCl) and the long-time oxygen evolution without attenuation indicate that the In2O3 truncated octahedrons are promising for photocatalytic oxygen evolution, and our results provide evidence that crystal cutting plays an important role in photofunctionization of materials. Sample Preparation: Indium oxide (In2O3) nanostructures were fabricated using a standard chemical vapor deposition (CVD) instrument. Indium oxide and graphite powders were mixed to a certain percentage (mass ratio = 1.5:1), ground, placed on an prepared alumina boat, and inserted into the CVD chamber. A gas mixture containing 98% of high-purity Ar and 2% of high-purity O2 served as the carrier gas and the pressure was maintained at 1 atm during the nanocrystal growth. A single-crystal n-type silicon wafer (<100> oriented, 0.5 mm thick, 1–10 Ω cm resistivity) was cut into smaller 8 mm × 10 mm pieces and used as the substrate. A thin layer of gold (10 nm) was predeposited on the silicon substrate by sputtering. The substrate was positioned downstream of the source and the furnace was heated from room tempearture to 1000 °C at a rate of 50 °C min−1 and a gas flow of 150 sccm. When the furnace temperature reached 950 °C, the truncated octahedrons were obtained and deposited for 3 h at the same gas flow of 150 sccm to obtain the corresponding sample. When the furnace was heated to 1000 °C, the octahedrons were obtained at a gas flow 100 sccm and deposited for 3 h (Supporting, Information, Figure S7). By adopting the aforementioned growth control, the thickness of the octahedron and truncated octahedron samples obtained by a Zeta 20 (Zeta Instruments, United States) was almost the same (22.7 μm) (Supporting Information, Figure S8). Characterization: The In2O3 nanocrystal structures were determined by XRD (Philips, Xpert) and the nanocrystal sizes and surface morphology were examined by FE-SEM (Hitachi, S4800). The photo-electrochemical measurements were performed on a three-electrode cell connected to a CHI 660D work station (CH Instrument) at ≈25 °C. On the backside of the Si substrate, an Ohmic contact was established by embedding a coiled Cu wire in a eutectic gallium-indium alloy (Aldrich) that wetted the silicon. The Cu wire and the eutectic alloy were subsequently covered with silver paint (SPI supplies). The silver layer in contact with the Cu wire was used as working electrode and it was not immersed in the electrolyte, whereas Ag/AgCl (1 mol L−1 NaOH-filled) and a platinum wire served as the reference and counter electrodes, respectively. The electrolyte was a 1 mol L−1 NaOH solution (pH = 13.6) and a 500 W Xe lamp served as the light source in the photo-electrochemical measurements. The lamp gave out directional light with uniform intensity distribution. The light was filtered to simulate the solar spectrum before illuminating the sample. A water filter (Supporting Information, Figure S9) between the lamp and electrochemical cell was used for eliminating the long-wave part of the radiation during the photocurrent measurement. It also reduced heating of the sample and the electrolyte, caused by the irradiation. The light power illuminating the sample was measured using a Si photodiode as being 270 mW cm−2. During the photocatalytic oxygen-evolution reaction, the amperometric I−t data were acquired from the electrochemical cell. The applied voltage was fixed at 0.22 V (versus Ag/AgCl). Oxygen Measurement: The oxygen measurement was conducted in a manner similar to the photocurrent measurement. Before the measurement, the anode was purged with highly pure N2 (99.9995%). When the electrode was irradiated, the chromoampometric test was begun at +0.22 V vs. reversible hydrogen electrode (Ag/AgCl) (RHE) for 150 min with O2 bubbling on the anode. 0.8 mL gas was taken from the headspace of the photoanode every 30 min and injected into a gas chromatography machine (Shimadzu GC-8A, Ar carrier gas) to determine the O2 concentration. This was then correlated to the total amount of O2 in the headspace. The amount of O2 in the solution was corrected using Henry's Law. Supporting Information is available from the Wiley Online Library or from the author. This work was supported by the National Basic Research Programs of China under Grants Nos. 2011CB922102 and 2013CB932901. Partial support was also provided by the National Natural Science Foundation (Nos. 60976063 and 61264008) and the Hong Kong Research Grants Council (RGC) General Research Funds (GRF) CityU 112510. As a service to our authors and readers, this journal provides by the Such materials are and may be for but are not or support from should be to the The is not responsible for the or of by the should be to the corresponding for the
28
Michel Armand, J.-M. Tarascon · Nature · 2008 · 19.3K citations
Co3O4 nanocrystals on graphene as a synergistic catalyst for oxygen reduction reaction
Yongye Liang, Yanguang Li, Hailiang Wang et al. · Nature Materials · 2011 · 5.4K citations · Full text