Temperature compensation of NdFeB permanent magnets

S. H. Kim, C. Doose

Proceedings of the 1997 Particle Accelerator Conference (Cat. No.97CH36167) · 2002 · 20 citations · 1 references

Concepts

Abstract

Permanent magnet blocks of NdFeB have a relatively high maximum energy product. Because of its relatively low Curie temperature, however, NdFeB has a large temperature coefficient for its residual induction. The temperature coefficients of the relative magnetic fields (/spl Delta/B/B)//spl Delta/T in the air gap of NdFeB dipole magnets were reduced from -1.1/spl times/10/sup -3///spl deg/C to less than 2/spl times/10/sup -5///spl deg/C under operating temperatures of /spl plusmn/6/spl deg/C. This was achieved passively by using 1.25-mm-thick strips of 30%-Ni-Fe alloy as flux shunts for the NdFeB blocks. The magnets with soft-steel poles and flux-return yokes were assembled and measured in a temperature-controlled environment.

References

1