IEEE Transactions on Applied Superconductivity · 2014 · 15 citations · 18 references
Natural SciencesMaterials SciencePhysicsCondensed Matter PhysicsNuclear MaterialsRadiation PhysicsAlloysMetallic Nuclear MaterialsMetalsRadiation Damage In MaterialsSuperconducting MaterialsCritical PropertiesCritical TemperatureIrradiation ConditionsMetal Radiation DamageRadiation-resistant Alloys
A recent proton irradiation study on Ta and Ti alloyed industrial multifilamentary Nb <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">3</sub> Sn wires has now been extended to fluences up to 1.38 × 10 <sup xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">21</sup> p/m <sup xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">2</sup> , the Bragg peak region being located outside of the wire. In the present work, magnetization measurements were performed up to 14 K and 10 T, to follow and determine with more precision the development of the upper critical field B <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c2</sub> with fluence. It was found that the critical temperature, T <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> , decreases linearly with increasing fluences, about 3% up to the highest fluence 1.38 × 10 <sup xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">21</sup> p/m <sup xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">2</sup> . The transition width does not change after irradiation, thus reflecting a homogeneous damage in analogy to neutron irradiation. Both the critical current density, J <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> , and the upper critical field, B <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c2</sub> , were found to increase in the considered fluence range. It was obtained that the larger enhancement of J <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> , (about 45% for Ta alloyed wires and 100% for Ti alloyed wires at 10 T) is not correlated to that of B <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c2</sub> (about 5% for Ti alloyed and 10% for Ta alloyed up to the highest fluence). The enhancement of J <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> in Ta alloyed wires is very similar for both PIT and RRP processing, thus assigning a major importance to the nature of the additive. The present results after irradiation were analysed applying the two-mechanism model on the volume pinning force, taking into account both grain boundary pinning and point pinning. A comparison between the present results and those achieved after neutron irradiation on the same Nb <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">3</sub> Sn wires shows that protons cause considerably higher damage than neutrons: the same effect on J <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> and T <sub xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">c</sub> is already observed at fluences being one order of magnitude smaller.
18
Flux pinning mechanisms in type II superconductors
D. Dew‐Hughes · Philosophical magazine · 1974 · 1.2K citations