Journal of the Physical Society of Japan · 2013 · 25 citations · 3 references
Natural SciencesMaterials SciencePhysicsCondensed Matter PhysicsMaterials PhysicsSolid State PhysicsAntiferromagnetismElectrical ConductivityMagnetic Properties Of SolidsMagnetic SusceptibilityPhase TransitionsThermoelectric MaterialsCharge-density Wave FormationCharge-density WavesCrystal Structure-property RelationshipsCurie-weiss LawHall ConductivityTetragonal LatticesThermoelectric Transport
EuGa4 and EuAl4 crystallize in the BaAl4-type tetragonal structure. The antiferromagnetic order was observed at 15 and 16.5K in EuGa4 and EuAl4, respectively.1,2) The magnetic susceptibilities in EuGa4 and EuAl4 well follow the Curie–Weiss law with effective moments of 7.97 and 8.02 B, respectively, which are consistent with the theoretical value of 7.94 B for a Eu-divalent electronic state.1,3) In the electrical resistivity and thermoelectric power measurements under pressure, a shoulderlike change was observed below about 100K at 1GPa in EuGa4. Moreover, a similar resistivity hump was observed below TCDW 1⁄4 140K at ambient pressure in EuAl4. The authors in Ref. 2 considered that this transition corresponds to the emergence of a charge density wave (CDW). In this study, we measured the magnetoresistance and Hall effect to clarify whether this is indeed based on CDW transition. Single crystals of EuAl4 were grown by the Al self-flux method. The transverse magnetoresistance and Hall resistivity were measured with an AC resistance bridge. The magnetic field H was applied along the [010] and [001] directions. The electrical current flow J was parallel to the [100] direction. Figure 1 shows a Kohler plot for the transverse magnetoresistance in the configurations of H k 1⁄2001 and J k 1⁄2100 . Kohler’s rule, i.e., = 1⁄2 ðHÞ ð0Þ = ð0Þ 1⁄4 fðH= ð0ÞÞ, holds when the temperature dependences of the scattering relaxation time are the same for all carriers. The = above 150K, namely, at 150, 160, and 200K, is well scaled on a single curve, which indicates that Kohler’s rule is satisfied above TCDW. On the other hand, the = below 140K deviates from Kohler’s rule, indicating that the carrier density and/or the scattering mechanism change below TCDW. In the two-band model, the transverse magnetoresistance and Hall resistivity are expressed as xx 1⁄4 ex hxð ey þ hyÞ þ ð exR 2 h þ hxReÞH ð ex þ hxÞð ey þ hyÞ þ ðRe þ RhÞH2 ; ð1Þ yx 1⁄4 ðRe hx hy þ Rh ex eyÞ þ ReRhðRe þ RhÞH 2 ð ex þ hxÞð ey þ hyÞ þ ðRe þ RhÞH2 H; ð2Þ where ei ( hi) and Re (Rh) are the resistivity along the i 1⁄4 xor y-direction and the Hall coefficient of the electron (hole) band, respectively.4) The Hall coefficient of each band is inversely proportional to the carrier density as Re 1⁄4 1=nee and Rh 1⁄4 1=nhe, where ne and nh are the electron and hole densities, respectively. The resistivity of each band is ei 1⁄4 1=ne eie ( hi 1⁄4 1=nh hie), where ei ( hi) is the mobility of the electron (hole). The transverse magnetoresistance increases quadratically, = H, for a compensated metal (ne 1⁄4 nh) at a high field limit (!c 1), whereas it tends to saturate for an uncompensated metal (ne 61⁄4 nh). Here, !c is the cyclotron frequency and is the scattering relaxation time. !c is roughly estimated using the relation = ð!c Þ2, which is obtained from the free-electron model. There is one EuAl4 unit in a body-centered tetragonal primitive cell. Considering that Eu is divalent, as proved by the magnetic susceptibility data,3) EuAl4 is a compensated metal with an even number of valence electrons. The experimentally obtained H-dependent magnetoresistance of up to = 2:5 10 2 (!c 0:16), shown as the solid curve in Fig. 1, reveals that EuAl4 is a compensated metal above TCDW. On the other hand, the = below TCDW gradually deviates at higher fields from the initial H dependence, as shown by the broken curve in Fig. 1 and the broken line in the inset of Fig. 1, at 100K. The deviation at 100K occurs at = 8 10 3 (!c 0:09). This behavior corresponds to the tendency toward saturation at higher fields, although the high field limit (!c 1) is not satisfied. Therefore, the transverse magnetoresistance indicates that EuAl4 is a compensated metal above TCDW and changes into an uncompensated metal below TCDW. The present experimental result and the hump of μ just below TCDW indicate that ne or nh starts to decrease below TCDW. Figure 2 shows the temperature dependence of the Hall coefficient RH determined at 0 T, shown by solid circles for H k 1⁄2010 and by solid squares for H k 1⁄2001 . The phase transitions at TCDW 1⁄4 140K and TN 1⁄4 14K are well observed. RH is temperature independent and negative above TCDW for both field directions. This means that the anomalous Hall coefficient, which is related to the magnetic susceptibility, is negligible in EuAl4. The negative RH for the compensated metal indicates e > h. The absolute value of RH increases with decreasing temperature below TCDW. The Hall resistivity is proportional to the magnetic field above TCDW, for example, at 200K, as shown in the inset of Fig. 2. On the other hand, the Hall resistivity gradually deviates downward from the linear field dependence with decreasing 0.06
3
Magnetic and Fermi Surface Properties of EuGa<sub>4</sub>
Ai Nakamura, Yuichi Hiranaka, Masato Hedo et al. · Journal of the Physical Society of Japan · 2013 · 66 citations